For EVA midsole and outsole foam, the working range is 1–3 phr (parts per hundred of rubber/plastic). The right point depends on your EVA grade, filler loading and foaming system:

  • 1–1.5 phr — midsoles where cushioning is the priority and abrasion just needs to pass spec.

  • 2–3 phr — outsole-heavy areas, heel zones and children's shoes where wear life drives warranty cost.

Run a small ladder trial (1 / 1.5 / 2 / 3 phr) and test rebound, density, DIN abrasion and compression set at each step. In most EVA systems the abrasion gain flattens above 3 phr, so there is no benefit in over-adding.

One practical note: add the agent in the first mixing stage so the siloxane disperses before foaming agents are introduced — late addition can leave undispersed specks.